All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 9.73
Wollastonite 31.70
Nepheline syenite 34.60
EPK Kaolin 11.43
Silica 12.54

Instructions

Published in "Low-fire to cone 3 Recipes," in the September 2018 issue of Ceramics Monthly.

The image shown here has multiple glazes on it.
This recipe has been recalculated from the original to fire to cone 3. Apply very thinly for the best transparency. I control the cooling of the kiln at a rate of 100° an hour between 1900° and 1400°F for the best satin surface. Natural cooling produces a bit more gloss.