All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 16.80
Strontium Carbonate 12.00
Wollastonite 6.40
Nepheline Syenite 24.00
Grolleg Kaolin 8.00
Silica 32.80

Instructions

Published in "Functional Glazes," in the Feb 2016 issue of Ceramics Monthly.

A mid-range clear glaze that holds colorants well.
For Turquoise, add 2.0 % Copper Carbonate.

For Medium Blue, add 0.1% Cobalt Carbonate and 2.0% Copper Carbonate.

For Yellow, add 4% Mason Stain 6404.