All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Calcined EPK Kaolin 25.00
EPK Kaolin 25.00
Alumina Hydrate 50.00

Instructions


For best results, I brush a thin coat on the interior of the soft-brick molds that I use to cast solid chunks of glaze. It also works well on kiln shelves.

This recipe was shared bu Alex Zablocki in the March 2020 issue of Ceramics Monthly.