All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Strontium Carbonate 10.00
Talc 2.00
Ferro Frit 3124 27.00
Nepheline Syenite 30.00
EPK Kaolin 13.00
Silica 18.00
Add Amount
Light Rutile 9.00
Copper Carbonate 1.00

Instructions


This glaze was formulated by Matt Kelleher. Apply by dipping. It is a deep, opaque turquoise. In oxidation it is grassy green and a brighter green over white slip. It is very stable, not runny, with a satin feel.

This recipe was shared bu Julie Crosby in the June/July/August 2020 issue of Ceramics Monthly.