All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Manganese Dioxide 39.39
Cedar Heights Redart Clay 52.53
OM4 Ball Clay 4.04
Silica 4.04
Add Amount
Copper Carbonate 4.04
Copper Oxide 4.04

Instructions

Published in "Montana Glazes," in the Jan 2016 issue of Ceramics Monthly.

This glaze will run and pool if applied too thickly. This Glaze is not food safe.
Apply three coats with a brush or only two coats if using a spray gun.