All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 2.06
Dolomite 5.53
Talc 3.08
Whiting 1.73
Custer Feldspar 38.03
Cedar Heights Redart 40.12
Kentucky Ball Clay 9.46
Add Amount
Red Iron Oxide 4.50
Rutile 1.00

Instructions

Pictured with two coats of John’s SG-12, one coat Candace Black, and one coat of Hamada Rust, fired to cone 10 oxidation.

Published in "Oil-Spot and Hare's Fur Glazes" by John Britt, in the May 2011 issue of Ceramics Monthly.