All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldspar 41.90
Silica 26.20
Dolomite 8.70
Ferro Frit 3134 8.70
Whiting 8.40
Barium Carbonate 4.40
Zinc Oxide 1.70
Add Amount
Tin Oxide 2.60
Bentonite 1.00
Copper Carbonate 0.50

Instructions

Published in "Copper Oxide" by John Britt, in the Jun/Jul/Aug 2012 issue of Ceramics Monthly.