All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 0.99
Talc 14.85
Cedar Heights Redart 15.35
Cedar Heights Goldart 12.38
Newman Red Substitute 31.68
Hawthorn Fireclay 12.38
OM 4 Ball Clay 12.38
Add Amount
Fine Grog 11.88
Medium Grog 7.92

Instructions

Originally published in the May 2018 issue of Ceramics Monthly.
Add four rolls of toilet paper per 1 batch of clay. Tear up and mix the paper into hot water, then mix well until it breaks down into a pulp.