All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Petalite 17.80
Wollastonite 20.30
Ferro Frit 3134 21.20
EPK Kaolin 22.50
Silica 18.20
Add Amount
Uncalcined Zinc Oxide 7.90
Cobalt Carbonate 0.50

Instructions

Published in "Incised and Inlaid Tumblers," in the September/October 2018 issue of Pottery Making Illustrated. This recipe has been used by Andy Bissonnette.