All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 20.00
Custer Feldspar 45.92
Cornwall Stone 21.43
EPK Kaolin 12.65
Add Amount
Manganese Carbonate 0.26
Rutile 3.06
Bentonite 2.04

Instructions

Published in "Atmospheric Glazes" by Lisa York, in the Dec 2015 issue of Ceramics Monthly. The image shown here is the Honey Celadon glaze on top of Lisa York's Flashing Slip recipe. The orange-peeled grey areas in the image are just the Flashing Slip.
Do not apply thick or it may shiver or become runny.