All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 28.00
Ferro Frit 3195 23.00
Nepheline Syenite 4.00
EPK Kaolin 28.00
Silica 17.00

Instructions


This is the base glaze I use on my cup forms. I add colorants to achieve the yellow and blue-gray tones, and use a thick application to achieve the dripping effects. The glaze comes from Mastering Cone 6 Glazes by John Hesselberth and Ron Roy (page 89).

This recipe was shared by Branan Mercer in the September 2019 issue of Ceramics Monthly.