All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 2.80
Hibiscus Ash 46.30
Whiting 9.30
Feldspar 18.50
Nepheline Syenite 4.60
Kaolin 4.60
Silica 13.90
Add Amount
Bentonite 5.00
CMC Gum (per 1000g) 2.00

Instructions

Published in "Sandy Vitarelli" by Lynn Young and Jennifer Owen, in the Jan 2012 issue of Ceramics Monthly.