All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 13.21
Whiting 13.21
Ferro Frit 3134 19.73
Nepheline Syenite 19.73
EPK Kaolin 10.80
Silica 23.32

Instructions

Published in "Exploring Glazes: From Perfect fit to Crackle and Matte," in the March 2016 issue of Ceramics Monthly.

The piece in the image shown here has multiple glazes on it, including Hensley Matte sprayed over Smokey Green, resulting in an emerald color.
This glaze is best used in combination with other glazes rather than on its own. Use sparingly: I spray a thin, whispy layer.