All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 20.00
Ferro Frit 3134 20.00
Custer Feldspar 20.00
EPK Kaolin 20.00
Silica 20.00

Instructions


A clear glaze that will work well in oxidation and reduction. I use it very thin at a specific gravity of 1.32. If applied too thinly, the glaze will be a rough white. Applied too thick, it will be gray.

This recipe was shared by Nathan Willever in the May/June 2019 issue of Pottery Making Illustrated.