All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Cryolite 0.60
Nepheline Syenite 55.40
Low-Melt Spodumene 18.00
McNamee Kaolin 26.00
Add Amount
Veegum T 1.00

Instructions

White where thick; red where thin. Yields a very soft and fat surface with crawling. Crawls more strongly if fired soon after glazing.

Published in "Shinos in the Fire...An Odyssey with a Doorless Fiber Kiln" by Hank Murrow, in the Sept 2001 issue of Ceramics Monthly.
Best with early reduction and a long, concluding period of oxidation, or an oxidation soak during cooling.