All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 54.90
Talc 14.60
Silica 30.50
Add Amount
Red Iron Oxide 22.00

Instructions

 

Variable glaze. Results differ drastically depending on glaze application, thickness, firing and cooling speeds, type of kiln, kiln-brick thickness, what type of socks you are wearing, and a thousand other reasons.

Published in "Mid-Range Glazes" by Forrest Sincoff Gard, in the April 2017 issue of Ceramics Monthly.