All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 20.00
Custer Feldspar 30.00
EPK Kaolin 20.00
Silica 30.00
Add Amount
Red Iron Oxide 1.50

Instructions

Published in "Goblet with Elegance" by Yoshi Fujii, in the Jan/Feb 2015 issue of Pottery Making Illustrated.

Glossy green celadon breaks over texture.
Mix all dry ingredients together before adding water. Sieve through an 80-mesh screen to break up clumps and disperse colorants.