All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 10.00
Wollastonite 20.00
G-200 Feldspar 40.00
EPK Kaolin 10.00
Silica 20.00
Add Amount
Spanish Red Iron Oxide 1.00

Instructions

Published in "Blending the Lines" by Kenyon Hansen, in the Jul/Aug 2014 issue of Pottery Making Illustrated.
Crystal growth in this glaze is very sensitive to variations in cooling.