All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 2.00
Lithium Carbonate 4.00
Whiting 5.00
Nepheline Syenite 70.00
OM4 Ball Clay 14.00
Silica 5.00
Add Amount
Cobalt Carbonate 1.00
Rutile 2.00

Instructions

Published in "Cone 6-10 Glazes" in the Jan 2015 issue of Ceramics Monthly.

Matte kelly green where thin and very shiny blue with crazing where thick.
Mix all dry ingredients together prior to adding the water.