All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 18.00
Whiting 16.00
Custer Feldspar 40.00
EPK Kaolin 10.00
Silica 16.00

Instructions

Originally published in the May 2018 issue of Ceramics Monthly.