All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 26.40
Gerstley Borate 13.20
Lithium Carbonate 8.60
Magnesium Carbonate 35.00
EPK Kaolin 15.20
Silica 1.60
Add Amount
Zircopax 6.00
Mason Stain 6374 Turquoise 5.00

Instructions

This recipe was originally published in the January/February 2018 issue of Pottery Making Illustrated.
The fit of this glaze is tight, with no peeling up. The pattern is interesting, random, and the glaze is very hard. There is a small bit of sparkle. Not food safe.