All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 4.60
Dolomite 13.60
Lithium Carbonate 4.60
Red Iron Oxide 9.10
Unispar 22.70
Bentonite 1.80
OM4 Ball Clay 20.90
Silica 22.70

Instructions

The glaze is a minor modification of the glaze GA16 from Michael Bailey's Cone 6 Glazes, poured thick on Georgies Ceramic Supply's G mix 6 clay body.

Published in "The Many Faces of Iron: An Exploration in Cooling" by Dr. Carol Marians, in the Jun/Jul 2007 issue of Ceramics Monthly.