All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 6.70
Gerstley Borate 14.00
Whiting 8.60
Kona F-4 Feldspar (substitute Minspar 200) 47.20
EPK Kaolin 2.60
Silica 20.90
Add Amount
Zinc Oxide 6.70
Mason Stain 6315 6.30
Copper Carbonate 2.00

Instructions

Shown here as the green accent color on this pot.

Published in "Finishing Details" by Lindsay Scypta, in the Dec 2014 issue of Ceramics Monthly.
I brush this glaze on certain parts of a pot, then cover it with a matte glaze. This glaze will cause the matte glaze to flux and run, so be careful to allow for that running. I usually build a significant foot rim to catch drips. Test on a tile with a drip catch first!