All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 20.00
Hawthorne Bond Fireclay 80.00

Instructions

Published in "Atmospheric Glazes" by Lisa York, in the Dec 2015 issue of Ceramics Monthly. The image shown here is the Flashing Slip recipe on porcelain with Honey Celadon glaze over the Flashing Slip in some areas.
Mix to the consistency of very thick cream. Apply in a thin layer to leather-hard clay. Ball mill for 24 hours to break down the particle size of the Hawthorne Bond Fireclay.