All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
G-200 Feldspar 10.00
Spodumene 30.00
Pyrax (HS) 10.00
Fire Clay (Hawthorne) 25.00
OM4 Ball Clay 25.00
Add Amount
Red Iron Oxide* 1.75
Grog (48 mesh) 5.00

Instructions

Published in "Flameware" by David Pier, in the May 2011 issue of Ceramics Monthly.
*Add: Red Iron Oxide - 1.75% - 2%

Note: No guarantee is made by the author or CeramicRecipes.org regarding these recipes. All individuals must test materials and maintain quality control to ensure proper performance of any clay body - particularly flameware. To test if you actually have flameware after you fire it, don full protective clothing including a mask with a face shield and apply a propane torch flame directly to one spot on the test piece.  Once it gets red hot, pick it up with tongs and drop it in a metal bucket of water. If it can take that, then it is flameware. You still need to be careful because you can never be sure there aren't any pores that may create steam pressure in the future.