All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 18.70
Lithium Carbonate 6.50
Soda Feldspar (Minspar 200) 9.40
Alberta Slip (Albany Slip Substitute) 56.10
Silica 9.30
Add Amount
Superpax (Zircopax) 9.40
Tin Oxide 4.70
Cobalt Carbonate 2.00

Instructions

Published in "Re-coloring a Classic" by Deklan Ranlett, in the May/June 2012 issue of Pottery Making Illustrated.