All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 5.00
Dolomite 25.00
Lithium Carbonate 2.00
Strontium Carbonate 9.00
Ferro Frit 3134 10.00
Kentucky Ball Clay (OM 4) 24.00
Cedar Heights Redart 23.00
Silica 2.00

Instructions

This is a beautifully variegated fake ash glaze. It is a brighter yellow on porcelain with hints of green where thicker and terra cotta-colored where thin. It is not stable because it is low in silica, but to alter it would change the ash effect. While it does not meet strict requirements of stability, I use it anyway because I substituted strontium for barium.

Published in "Glaze Forward" by Diana Pancioli, in the June 2006 issue of Ceramics Monthly.