All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 10.88
Whiting 11.92
Custer Feldspar 25.39
EPK Kaolin 24.35
Silica 27.46
Add Amount
Zinc Oxide 3.63

Instructions


A Bomb-proof glaze developed to reduce crazing and bubbles on the Bomb-Proof White Tile Body. This incredibly durable oxidation glaze is perfect for tile and works particularly well with Mason stains.

This recipe was shared by Forrest Lesch-Middelton in the October 2020 issue of Ceramics Monthly.