All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Spodumene 4.00
Talc 4.00
Zinc Oxide 27.00
Ferro Frit 3110 50.00
Silica 15.00
Add Amount
Manganese Dioxide 1.00
Titanium Dioxide 1.00

Instructions

Published in "Gemstones & Glazes" by Ryan Coppage, in the Sep 2017 issue of Ceramics Monthly.

This glaze runs. It also forms small crystals that can be further developed with a more complex firing schedule.