All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 9.50
Ferro Frit 3124 (sub. JM Frit 169) 44.50
Custer Feldspar (sub. Forshammer) 20.00
EPK Kaolin 5.00
Silica 8.00
Add Amount
Tin Oxide 9.00
Red Iron Oxide 3.00
Bentonite 7.50

Instructions


Specific gravity: 1.40. Eggshell glaze has a strong breaking white effect against a glossy rust background. I substituted Forshammer feldspar for Custer Feldspar due to availability, and used JM frit 169 in place of Ferro frit 3124 in this glaze. These frits are not similar. JM frit 169 has no alumina and includes barium.

Original recipe shared by Central Carolina Community College in the October 2004 issue of Ceramics Monthly.

This recipe was shared by Alisa Clausen in the February 2020 issue of Ceramics Monthly.