All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 16.00
Ferro Frit 3124 42.00
Nepheline Syenite 16.00
OM 4 Ball Clay 18.00
Silica 8.00
Add Amount
CMC Gum 0.50

Instructions


This is a glossy base that works well with ceramic stains and coloring oxides. Substitute all or part of the wollastonite with dolomite to create a satin to satin-matte surface.

This recipe was shared by Marc Egan in the September/October 2020 issue of Pottery Making Illustrated.