All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 19.80
Ferro Frit 3124 19.80
Nepheline Syenite 19.80
EPK Kaolin 19.80
Silica 20.80
Add Amount
Bentonite 2.00
Mason Stain (for color) 5.00

Instructions

This recipe was published in the May/June 2018 issue of Pottery Making Illustrated. This glaze originally came from Eric Mirabito. The surface is responsive to rates of cooling in the kiln.
Cool slowly for a true satin-matte surface. Fast cooling will show the glossier side of this glaze.