All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 19.80
Ferro Frit 3124 19.80
Nepheline Syenite 19.80
EPK Kaolin 19.80
Silica 20.80
Add Amount
Bentonite 2.00

Instructions


I apply this glaze by spraying, then cool the kiln slowly at the end of the firing to achieve a satin surface. Original recipe attributed to Eric Mirabito, shared with me by Chandra DeBuse.

This glaze was shared by Stephanie Wilhelm in the November 2019 issue of Ceramics Monthly.