All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 1.02
Talc 7.11
Whiting 22.34
Custer Feldspar 31.47
EPK Kaolin 12.68
Silica 25.38
Add Amount
Mason Stain #6440 1.50

Instructions

Published in "Cone 6-10 Glazes" in the Jan 2015 issue of Ceramics Monthly.

I fire this to cone 9. This glaze has a satin surface at cone 8. It is a good base for experimenting with colorant additions.
After mixing, sieve the glaze through at least an 80-mesh screen to remove lumps and disperse any colorants evenly.