All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 14.73
Custer Feldspar (sub. Forshammer) 46.90
Georgia Kaolin (or EPK) 8.34
Silica 30.03
Add Amount
Tin Oxide 4.33
Titanium Oxide 4.33
Zinc Oxide 8.24
Bentonite (omitted) 3.25

Instructions


Specific gravity: 1.43. This glaze is opaque and glossy, but has a soft sheen on the surface. Many color variations were possible, all of which are opaque, bright, and clean. For color variations, omit the tin oxide, titanium dioxide, and zinc oxide. I substituted Forshammer feldspar for Custer feldspar.

Original recipe shared by Gerald Brown in the June 1991 issue of Ceramics Monthly.