All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 25.00
Ferro Frit 3134 15.00
Silica 20.00
Sand (50-mesh) 5.00
Tennessee Ball Clay #1 25.00
Anhydrous Borax 3.00
Soda Ash 4.00
Bentonite 3.00
Add Amount
Cobalt Carbonate 1.00

Instructions

Published in "Egyptian Paste" by Robin Hopper, in the Jul/Aug 2010 issue of Pottery Making Illustrated.
Mix well and sieve to 60-mesh or finer while dry. Add a small amount of water and mix to a dough-like consistency.