All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3195 45.00
Ferro Frit 3134 30.00
EPK Kaolin 25.00
Add Amount
Mason Zirconium Yellow 2.00

Instructions

This is a shiny, transparent glaze that is very responsive to colorants. Without colorants, it is food safe. With colorants, you'll need to have it tested for leaching those colorants.

Published in "Polychrome Glazes" by Joan Bruneau, in the April 2014 issue of Ceramics Monthly.
Apply thin in order to ensure the fired glaze will be a transparent clear. Use a thicker application with colorants to achieve a rich translucent glaze. Use 2–6% Mason stain.