All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 19.89
Custer Feldspar 34.81
EPK Kaolin 14.92
Silica 30.38
Add Amount
Zinc Oxide 4.74
Celadon MS 6201 0.98

Instructions

Published in "Atmospheric Recipes," in the October 2018 issue of Ceramics Monthly. This recipe has been used by Susan McKinnon.
Add a pinch of Epsom salts to the glaze to improve consistency. Tone will vary for each of the Mason stains (MS) with different atmospheres. In reduction, the green is brighter but in oxidation it is an olive shade. In oxidation, the blue is very pale, but in reduction the color is brighter.