All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 21.05
Custer Feldspar 47.37
EPK Kaolin 10.53
Silica 21.05
Add Amount
Red Iron Oxide 3.16
Cobalt Carbonate 2.11

Instructions

This recipe was shared by Hanako Nakazato in the June/July/August 2018 issue of Ceramics Monthly.