All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3110 100.00
Silica 4.00
EPK 6.00
Add Amount
Silver Nitrate 2.00
Bismuth Nitrate 4.00
Cobalt Carbonate 4.00

Instructions

This glaze is from Greg Daly's book, Lustre.

The test tile is B-Mix, fired in oxidation and re-fired in a reduction atmosphere.


This glaze needs to have a post-fire reduction to get its incredible iridescence.  Blue stripe on test tile is acid-etched.  Original recipe called for cobalt oxide but cobalt carbonate was substituted.