All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 10.31
Whiting 10.31
Nepheline Syenite 40.24
EPK Kaolin 7.22
Silica 31.92
Add Amount
Bentonite 1.00

Instructions

Reliable, stable, clear/glossy base glaze that holds colorants well. Try testing this base with the addition of other oxides, carbonates, and commercial stains to achieve different colors.

Published in "Mid-Range Glazes" by Forrest Sincoff Gard, in the April 2017 issue of Ceramics Monthly.
Interesting results, glaze movement, and deeper colors can be achieved when glazes made with Dale Huffman's Clear and Matte Clear glaze combinations can run and are not as stable, so always test and use with caution.