All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 18.00
Wollastonite 11.00
ZInc Oxide 14.00
Minspar 200 Feldspar 44.00
EPK Kaolin 6.00
Silica 7.00
Add Amount
Veegum T 2.00

Instructions


The added Veegum T makes this glaze very brushable, which is often my preference.

I use D-Base glaze on the exterior of all my pots.

This glaze is fired to cone 8 in oxidation, but can be fired from con 6–8. It works best when applied thin, about the consistency of 1% milk. I always sieve and mix thoroughly before applying.

This glaze was shared by Doug Peltzman in the December 2019 issue of Ceramics Monthly.