All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 90.91
Edgar Plastic Kaolin 9.09
Add Amount
Zircopax 13.64

Instructions

Shown here on work by Woody Hughes.

Published in "Val Cushing's Glazes" in the Apr 2014 issue of Ceramics Monthly.