All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Liquid Wax Emulsion 50.00
Ferro Frit 3124 3.00
Red Iron Oxide 5.00
Black Iron Oxide 5.00

Instructions


Measurements in grams. Thoroughly wet the oxides with a few drops of water before adding the wax. Mix ingredients, then pass through an 80-mesh sieve to remove lumps. Clean the sieve with hot water and dish soap immediately after using.

This recipe was shared by Marc Egan in the September/October 2020 issue of Pottery Making Illustrated.