All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 29.00
Custer Feldspar (sub. Forshammer) 40.00
Spodumene 4.00
EPK Kaolin 27.00
Add Amount
Cobalt Carbonate 2.00

Instructions


Specific gravity: 1.43. A calcium matte with a hard and flat surface. The color tests showed a neutral color response; however, the red iron oxide showed some variegation with yellows on a rust ground. I substituted Forshammer feldspar for Custer feldspar.

From Pottery Making Illustrated.

This recipe was shared by Alisa Clausen in the February 2020 issue of Ceramics Monthly.