All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 28.00
Nepheline Syenite 46.00
EPK Kaolin 6.00
Silica 20.00
Add Amount
Bentonite 1.00

Instructions


The source of this recipe is unknown. Apply a thin coat for best results. Use a dry finger to smooth any pinhole-like marks on the surface before firing. This stable glaze has a softer shine than the high-gloss found in many clear glazes. I fire it to cone 1 with a 10-minute hold in an electric kiln.