All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Continental Clay's Domestic Porcelain 50.00
Laguna Clay's Babu Porcelain 50.00
Add Amount
Mason Stain 6531 Slate 8.00
Mason Stain 6540 Blue Gray 2.00

Instructions

Originally published in the May 2018 issue of Ceramics Monthly.
To mix, start with a slurry of porcelain base (a mixture of two commercial clays) and slowly add stain mixture. Dry to desired consistency on plaster slabs. In oxidation, lower temperatures for a lighter, higher temperature for more a saturated tone. Stains can be used with any porcelain, reclaim makes a great base.