All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 20.00
Ferro Frit 3249 20.00
Nepheline Syenite 20.00
Glomax LL 15.00
Silica 25.00

Instructions


Glomax LL is a calcined kaolin. For best results, keep the specific gravity of the mixed glaze between 1.2–1.4, as a thick application will crawl.

This recipe was shared by Kyle Johns in the June/July/August 2020 issue of Ceramics Monthly.