All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldspar 25.00
6Tile Kaolin 30.00
OM 4 Ball Clay 20.00
Silica 25.00
Add Amount
Best Black 6600 Mason Stain 10.00

Instructions


Mix 2 teaspoons of Darvan #7 (deflocculant) into 12 ounces of hot water. Mix into dry ingredients, adding in more water as needed to achieve a thick, cream-like consistency.

This recipe was shared Dodie Campbell in the May/June 2021 issue of Pottery Making Illustrated.