All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 13.46
Zinc Oxide 11.54
Soda Feldspar (Minspar 200) 36.54
Ball Clay 5.77
Silica 32.69
Add Amount
Copper Carbonate 0.58

Instructions

Published in "Working Potter Glazes" in the June 2015 issue of Ceramics Monthly.

Chun (light green) is a very stable glaze used as a liner. If thick, it can craze, but it does not run. Can be thinned when layering glazes. This glaze has a wide temperature range.
Mix all ingredients together prior to adding the water.